1) Pressing the electrode, pressing the sponge titanium through a press to form a dense sponge titanium pressed block electrode;
2) Vacuum casting, under vacuum conditions of 1700 to 1800 ° C and -103Pa, perform three times of vacuum casting on the sponge titanium compact electrode;
3) Opening, under the condition of 1000 ℃, open the blank through an oil press, and finally press it into a square blank;
4) The first rolling, under the condition of 970 ~ 980 ℃, preliminary rolling into a cylindrical shape blank with a rolling mill;
5) The second rolling, under the condition of 950 ° C, is rolled into a blank by a rolling mill.
grade 2 titanium bar grade 2 titanium wire titanium seamless pipe thin wall titanium tube
2) Vacuum casting, under vacuum conditions of 1700 to 1800 ° C and -103Pa, perform three times of vacuum casting on the sponge titanium compact electrode;
3) Opening, under the condition of 1000 ℃, open the blank through an oil press, and finally press it into a square blank;
4) The first rolling, under the condition of 970 ~ 980 ℃, preliminary rolling into a cylindrical shape blank with a rolling mill;
5) The second rolling, under the condition of 950 ° C, is rolled into a blank by a rolling mill.